About Factory Quality FAQ Blog Contact
Get a Quote WhatsApp
Technical Guide · 9 min read

PCE Dosage per kg of Cement: The Formula, the Ranges, the Mistakes

Dosage is never just one number. How to calculate PCE addition from binder weight, convert between liquid and solid, and adjust for what actually moves the figure.

Published 3 November 2026 · by the PCE Additive technical team

Ask five suppliers for a PCE dosage and you will get five numbers, usually somewhere between 0.1% and 1.0%. All of them may be right — for their own product, their own basis and their own test mix. The number only means something once you know what it is a percentage of, whether it is quoted on a liquid or solid basis, and which variables in your mix move it.

This is the calculation we walk customers through every week, with worked examples you can copy into a batching sheet.

The formula, stated properly

Dosage is nearly always expressed as a mass percentage of cementitious binder:

Dosage (%) = mass of admixture as supplied ÷ mass of binder × 100

The two words that cause most arguments are "as supplied" and "binder".

  • As supplied means the liquid you pour from the drum, water included — not the dry polymer. A 50% solid liquid dosed at 0.4% delivers only 0.2% active polymer.
  • Binder may mean cement only, or cement plus fly ash, slag and silica fume. On a 350 kg binder containing 30% fly ash, the difference between the two conventions is 30% of your dose. Always ask which basis a supplier used.

Worked example: one cubic metre of ready-mix

Mix design: 300 kg CEM I 42.5 + 50 kg fly ash (350 kg binder), target C35, ambient 25 °C, 45-minute haul. Your lab trial found 0.22% of a 50% solid liquid to be the sweet spot.

StepCalculationResult
Admixture per m³350 kg × 0.22%0.77 kg
Active polymer0.77 kg × 50%0.385 kg
Dosage on cement only0.77 ÷ 300 kg0.257%
Per 1,000 kg of binder1,000 × 0.22%2.2 kg
Per 100 kg batch (lab)100 × 0.22%0.22 kg = 220 g

Note the third row: the same mix is "0.22%" or "0.257%" depending on whether fly ash counts as binder. Both are honest; only one matches your batching system's convention. Agree on it in writing with your supplier before the first container ships.

Typical dosage ranges by application

ApplicationFormDosage (% of binder, as supplied)
Ready-mix, C25–C40Liquid 40–50%0.15 – 0.25%
Ready-mix, C50 and aboveLiquid 50–60%0.25 – 0.45%
Self-compacting concreteLiquid 50–60%0.30 – 0.60%
Precast, fast demouldingLiquid 50%0.20 – 0.40%
Dry-mix mortar, tile adhesivePowder ≥ 95%0.10 – 0.30%
Self-levelling (SAC / gypsum)Powder ≥ 95%0.15 – 0.35%
UHPCPowder or liquid0.80 – 1.50%
Low-cement refractory castablePowder0.05 – 0.20%

These are starting points for trials, not specifications. A C50 mix with 40% slag and a 90-minute haul can legitimately need twice the dosage of a plain C50 mix poured on site.

Converting between liquid and powder

Because the two forms are quoted on wildly different solid contents, a direct percentage swap will be wrong by a factor of two or more. Normalise to active polymer first:

Liquid dosage (as supplied)Solid contentActive polymerPowder equivalent (≥ 95% solid)
0.20%40%0.080%0.084%
0.25%50%0.125%0.132%
0.30%50%0.150%0.158%
0.40%60%0.240%0.253%

In practice you will usually need slightly more powder than the arithmetic suggests, because spray-dried polymer redisperses less perfectly than fresh liquid. Budget 5–10% extra and confirm by trial.

From mother liquor to working solution

Most plants buy 40–60% mother liquor and dilute to a 15–25% working solution so the dosing pump can meter accurately. To make a batch at target concentration:

Mother liquor (kg) = working solution (kg) × target % ÷ mother liquor %
Water to add (kg) = working solution (kg) − mother liquor (kg)

Example: 1,000 kg of 20% working solution from 50% mother liquor needs 400 kg liquor plus 600 kg water. Two practical notes: use clean water (hard water can precipitate the polymer), and stir while adding — dumping liquor into water creates lumps that take hours to dissolve. See our liquid mother liquor grades for the solid contents we supply.

Five variables that move the number

VariableEffect on dosageRule of thumb
Cement C3A content and finenessHigher C3A and finer grinding adsorb more polymer+10–30% versus a low-C3A cement
SCMs (fly ash, slag, silica fume)Fly ash and slag: slight increase. Silica fume: large increaseSilica fume above 5% often needs +20–40%
TemperatureHot concrete loses workability faster and adsorbs polymer quickerAbove 30 °C, expect +10–20% or add a retarder
Aggregate claySwelling clays consume PCE side chainsUse an anti-clay grade rather than dosing up
Water content and paste volumeHigher w/c dilutes the effect; richer mixes need more per m³Always dose against binder, never against total mass

Overdose: what it looks like and how to recover

  • Bleeding and segregation — water separates, aggregate sinks. Recovery is difficult once placed; you can sometimes re-temper with a viscosity modifier, but the load is usually compromised.
  • Retarded set and dusting — the surface stays soft for hours and dusts under trowel. In precast this costs a full cycle.
  • Excess air — strength drops roughly 5% for every 1% of entrained air beyond target.
  • Cost — and the cheapest fix is the boring one: cut the dose back to the trial value and re-check your aggregate moisture probe. Overdosing is almost always a moisture-measurement error, not a formulation decision.

Trial protocol before you commit

  1. Paste trial in the lab to bracket the range: 0.10%, 0.15%, 0.20%, 0.25%, 0.30%.
  2. Mortar or concrete trial at the two best points, with real aggregates at real moisture.
  3. Measure flow at 0, 30 and 60 minutes — not just at mixing.
  4. Cast cubes and test 1, 7 and 28 days.
  5. Plant trial of one full batch, watching discharge and 30-minute workability.
  6. Lock the number in your batching system, and re-verify whenever cement source or season changes.
Send us your mix design — binder composition, w/c, strength class, haul time and aggregate type — and we will come back with a recommended grade and a starting dosage for your trial. Our PCE is polymerised in Suzhou from our own monomers, so the grade you trial is the grade you receive in the container.

Ready to calculate? Send your mix design on WhatsApp and we will return a dosage recommendation within one working day. For the formulation side, see why more PCE is not better and our SAC admixture guide.

FAQ

Is PCE dosage calculated on cement or on total binder?

Both conventions exist. International suppliers usually mean total cementitious binder; many local plants mean cement only. On a mix with 30% SCM replacement the numbers differ by about 40%, so confirm the basis before comparing quotes or trial results.

How many kg of PCE per cubic metre is normal?

For a typical C30 ready-mix at 350 kg binder and 0.20% dosage, roughly 0.7 kg of 50% liquid per m³. High-strength and SCC mixes run 1.2–2.5 kg per m³. Anything above 4 kg per m³ suggests a formulation problem rather than a dosage one.

Can I dose PCE by volume instead of weight?

Only as a cross-check. Liquid PCE density varies with solid content (roughly 1.05–1.12 kg/L), so volume dosing drifts as soon as you change grade. Meter by weight or calibrate the pump against a weighed sample every shift.

Have a question this article did not answer?

Our technical team answers specific questions about dosage, cement compatibility and troubleshooting. Send yours and we will reply within 12 working hours — no obligation.

Chat on WhatsApp