Defoamer and Anti-Spalling Fibers for Refractory Castables

By the time the dispersant has pulled the water demand down, two things decide whether the lining survives its first heat-up: the air you mixed in and the water that is left. This guide covers both — how to get the air out before casting, and how to give the steam somewhere to go afterwards.

Published 18 November 2026 · by the PCE Additive technical team

Air and water are the two leftovers of every castable mix. The dispersant removes the water that placement does not need — that was the subject of the previous guide — but the air you mixed in and the water that remains still have to leave the lining, one before casting and one during the first heat-up. Get either wrong and the defect is from the same family: porosity, lost strength, and in the worst case a lining that fails explosively during dryout.

Why a low-cement mix holds its air

  • High-shear mixing. A heavy-duty mixer at full speed entrains air efficiently, and the finer the grading, the more of it stays.
  • Tight particle packing. The same densely graded fines that make a low-cement castable strong also trap bubbles between particles, where buoyancy alone will never move them.
  • High paste viscosity. At 4.5% – 7% water the paste is stiff; bubbles rise slowly or not at all.
  • Flow is not de-airing. A self-flow mix can reach its target spread diameter carrying 4% – 6% of entrained air. Flow measures where the mix goes, not what it left behind.

The cost is familiar: every additional percent of entrained air costs roughly 4% – 6% of cold crushing strength, pinholes and pits mark the cast face, and the porosity shows up again after firing. The first diagnostic is cheap and worth a permanent place on the batch card: weigh a known volume of fresh mix and compare its density with the theoretical value calculated from the formula. The gap is your air.

Defoamer chemistry and dose

TypeFormTypical doseNotes
Silicone (on mineral carrier)powder, dry-blended0.02% – 0.10% of dry massFast knockdown; overdose can leave a hydrophobic film that harms wetting and the cast face
Polyglycol / mineral oil basedliquid or on carrier0.02% – 0.10% of dry massSlower but gentler on the polymer; the safer default where a PCE dispersant is dosed
Specialty fluorinated gradesliquidcase by caseOnly where conventional chemistry fails; cost and regulatory burden are real

Placement follows the same logic as the dispersant. A powder defoamer is dry-blended with the cement and the fine fraction first — the same 60-second pre-blend rule as WT101 — and never tipped onto coarse aggregate. A liquid defoamer goes into the mixing water before the dry blend, so it acts as an antifoam from the first second of shear instead of chasing foam that already exists.

One interaction deserves its own paragraph, because it is the failure mode that gets misdiagnosed: a defoamer is a surfactant, and a PCE dispersant works by adsorbing on surfaces. Overdose the defoamer and it competes for the same interfaces, stripping polymer from the fines. The symptom is a mix that stiffens right after the defoamer goes in — which looks exactly like under-dosing the dispersant, and the instinctive response (more dispersant) makes it worse. The same competition is documented in well cementing slurries, where the dose ladder is better established: start low, increase in small steps, and record what fixed it (see the cement slurry defoamer guide for the detailed version).

What air costs, and how to measure it

  1. Theoretical density. Calculate it from the formula every time a raw material changes. Without this number, "the mix looks a bit light" is not a measurement.
  2. Fresh density against theoretical. A gap of 1% is normal; a gap of 2% – 3% is air you will pay for at 110 °C.
  3. Flow retention. Check flow again 30 minutes after mixing. A defoamer that fixes density but costs 15% of flow has moved the problem, not solved it.
  4. Cast face inspection after demould. Pinholes and pitting are the visible fraction of the air; assume the rest is in the body.

Explosive spalling: the mechanism

Dense low-cement castables have low permeability. During the first heat-up, free water evaporates at around 100 °C and steam pressure builds inside the section. If vapour cannot escape faster than it is generated, pressure rises until it exceeds the tensile strength of the still-green body — and a piece of the lining comes off explosively, usually between 150 °C and 350 °C, where bound water is also leaving.

The uncomfortable part is that the dispersant makes this worse, not better. Lower water means a denser, less permeable body, which is exactly what gives better hot strength — and exactly what makes it harder for steam to escape. Anti-spalling measures are not a legacy concern from wetter mixes; they scale up as water goes down. A 5% water lining with 0.2% dispersant is more exposed on first heat-up than a 7% water lining ever was.

Risk factors stack: thick sections, sealed formwork, fast ramps, and any area where the heating is applied from one face only.

Anti-spalling fibres: venting built into the body

FibreWhat it doesDoseNote
Polypropylene (PP)Melts at about 165 °C and leaves micro-channels for steam; expansion before melting opens the channels further0.05% – 0.15% of dry massThe standard anti-spalling choice; length 6 – 12 mm
Polyvinyl alcohol (PVA)Survives to roughly 230 °C; adds green strength as well as venting0.05% – 0.15% of dry massWhere demould strength and spalling protection are both wanted
Steel fibreDoes not melt or vent in this range—For mechanical toughness, not anti-spalling; do not count it in the venting budget

Fibre must survive mixing to work. Add it at the end of the dry blending — after cement, fines and dispersant are already homogeneous — and limit the high-shear stage after water to what the placement actually needs. Long high-shear mixing fibrillates and balls the fibre, and a balled fibre is a defect rather than a vent.

The dryout curve does most of the work

Fibres are a safety net, not a substitute for a disciplined first heat-up. A typical starting schedule for a dense low-cement body — to be adjusted to the specific product and section thickness:

  1. Ambient to 110 °C at no more than about 50 K/h.
  2. Hold at 110 – 150 °C until free water is gone — roughly one hour per 25 mm of section thickness as a starting point, longer for dense low-cement bodies.
  3. 150 °C to 350 °C at 25 – 50 K/h. This is the danger zone; nothing about the schedule matters more than this ramp.
  4. Hold at about 350 °C until bound water evolution tapers.
  5. Then to service temperature at the rate the lining design allows.

Two details that cost nothing: vent the formwork or leave weep holes, and never seal a thick section airtight while it dries. Most spalling incidents in the field are a fast ramp plus a sealed mould, with the fibre package blamed for not saving an undrained body.

Failure patterns and the first move

SymptomLikely causeFirst move
Pinholes and pitted cast faceAir not released; defoamer missing, wrong type or added lateDefoamer into the water or the dry pre-blend; verify fresh density
Fresh density 2% – 3% below theoreticalEntrained air from high-shear mixingAdd defoamer, extend the low-speed stage; recalculate theoretical density
Mix stiffens after defoamerDefoamer stripping PCE polymer — overdoseCut the defoamer dose; do not add dispersant on top
Explosive spalling at 200 – 300 °CPermeability too low, ramp too fast, section sealedPP fibre package, slower ramp through 150 – 350 °C, vent the formwork
Surface cracks on first heatThermal gradient too steep for the sectionSlower ramp, longer holds; check section thickness against schedule
Fibre balls in the mixFibre added too early or high-shear time too longAdd fibre last, in the dry stage; shorten the wet high-shear time

Test the blend, not the additives one by one

The three components in this guide interact: the dispersant lowers water, the lower water raises the spalling exposure, and the defoamer competes with the dispersant for interfaces. A lab result for any one of them alone predicts very little about the installed lining. The minimum set before the first production lining:

  • Fresh density against theoretical, at the production mixing energy.
  • Flow and flow retention at 30 minutes, with defoamer and dispersant at their intended doses.
  • A spalling test on 100 – 150 mm cubes heated at the site ramp — not a standard-rate oven curve that flatters the body.
  • Apparent porosity and MOR after 110 °C and at service temperature.

We supply the dispersant leg of this package — WT101 powder for refractory and high-alumina bodies — and we would rather you bought the defoamer and the fibre from whoever supplies them best, provided the three are tested together. Send the mix design, the placement method and the dryout schedule, and we will return a starting WT101 dose and the flow we expect at that dose; the refractory castable application page carries the grade summary.

Frequently asked questions

How much defoamer goes into a refractory castable?

0.02% – 0.10% of dry mass, starting around 0.05%. Powder silicone grades are dry-blended with the cement and fines first; polyglycol liquids go into the mixing water before the dry blend. Confirm the dose with fresh density against theoretical — that measurement, not the absence of visible foam, is the pass criterion.

How much polypropylene fibre prevents explosive spalling?

0.05% – 0.15% of dry mass at 6 – 12 mm length, added at the end of dry blending. Fibres are a vent, not a substitute for the dryout curve: the slow ramp through 150 – 350 °C and vented formwork are still mandatory, and most field spalling is a fast ramp plus a sealed mould.

Does a stronger dispersant increase spalling risk?

Indirectly, yes. Better dispersion means lower water, and lower water means a denser body with lower permeability — better hot strength, but harder steam escape on first heat-up. That is why anti-spalling measures should scale with water reduction, not stay at whatever the older, wetter mix used.

Silicone or polyglycol defoamer with a PCE dispersant?

Polyglycol or mineral-oil grades are the safer default with PCE-based dispersants. Silicone knocks foam down faster but is a more aggressive surfactant, and overdose can strip polymer from the fines and stiffen the mix. Whichever you choose, run flow and fresh density with the defoamer and dispersant at their production doses before committing a batch.

Have a question this article did not answer?

Our technical team answers specific questions about dosage, cement compatibility and troubleshooting. Send yours and we will reply within 12 working hours — no obligation.

Chat on WhatsApp